Concrete moisture testing before an epoxy floor coating in Kansas City is done with two measured tests, the calcium chloride test (ASTM F1869) and the in-slab relative humidity test (ASTM F2170), and the coating manufacturer's written limit decides whether the slab passes. A plastic sheet taped to the floor and a handheld meter can flag a problem, but neither one is a pass.
Why every slab is tested, even an old dry-looking one
A slab can look and feel dry and still be giving off a steady flow of vapor. The ASTM calcium chloride method starts from the fact that "all concrete subfloors emit some amount of moisture in vapor form" (ASTM F1869). Vapor emission simply means moisture leaving the slab as vapor. On bare concrete it escapes into the room unnoticed. Under a coating that does not breathe, it collects at the bond line.
The concrete industry counts epoxy among the moisture-sensitive floors. The American Concrete Institute's guide to slabs that receive moisture-sensitive flooring lists "epoxy coatings" alongside vinyl, rubber, carpet and wood (ACI PRC-302.2-22). And the ASTM relative humidity method notes that makers of floor systems generally require moisture testing before installation on concrete (ASTM F2170).
Where slab moisture comes from
The ready mixed concrete association lists five sources of moisture in a slab (NRMCA CIP 28):
- Ground water rising by capillary action through fine-grained soil.
- Water vapor from the soil. The humidity of the subgrade under a slab on ground "will measure close to 100%", wherever the building is.
- A wet fill layer under the slab.
- Mix water still held in the concrete.
- Water that gets on the slab during construction.
For a building owner, the second source is the one that never goes away. A slab on ground anywhere sits on damp soil. One of the association's main defenses is a vapor retarder directly beneath the slab, and an older building may have been built without one. No surface test can add a vapor retarder after the fact; testing can only tell you how much moisture is coming through.
The calcium chloride test (ASTM F1869)
What it measures: the rate of moisture vapor leaving the surface of bare concrete, stated in pounds of moisture over 1,000 square feet in 24 hours (ASTM F1869). It can be used on floors below grade, on grade and above grade.
How it is run, in the ready mixed concrete association's summary: a measured amount of calcium chloride salt sits in a dish sealed under a plastic dome on the slab, and the moisture the salt absorbs "in 60 to 72 hours" gives the emission rate (NRMCA CIP 28).
Where it does not apply: the ASTM method is not for gypsum concrete or floors with lightweight aggregate, and not for use over coatings, reactive penetrants, or patching or leveling compounds. It is a test of bare concrete.
Shortcomings the association names: it reads only shallow moisture near the surface, it is sensitive to the temperature and humidity of the room, and it is a snapshot.
The in-slab relative humidity test (ASTM F2170)
What it measures: the percent relative humidity inside a concrete slab, in the field or in a laboratory (ASTM F2170).
How it is run, in the association's summary: humidity is measured at a set depth inside a drilled or cast hole, after the hole has been left to reach equilibrium "for 72 hours" (NRMCA CIP 28).
What it adds: because it reads inside the slab rather than at the surface, it shows moisture the calcium chloride test cannot reach. The ASTM method explains why that matters, listing the failures excess moisture can cause after a floor goes down: "debonding, peaking and deterioration of finish flooring and coatings and microbial growth".
The plastic sheet test and moisture meters
The plastic sheet test is a screening check. In the association's summary, an 18 by 18 inch sheet is taped tight to the slab "for at least 16 hours". Moisture under the sheet is a positive sign of excess moisture, "however, a negative indication is not an assurance that the slab is acceptably dry below the surface" (NRMCA CIP 28). The ASTM method behind it describes it as a way to indicate capillary moisture, which "may be detrimental to the performance of certain coating systems" (ASTM D4263).
Electronic moisture meters are, in the association's words, "useful survey tools" that give comparative moisture readings across a floor. Neither the sheet nor the meter replaces a measured test.
What counts as a pass
The pass mark belongs to the coating manufacturer. The federal standard resinous flooring specification tells the installer to "verify that the concrete substrates are dry and the moisture-vapor emissions are within acceptable levels according to the manufacturer's written instructions" (UFGS 09 67 23.13). Published reference points show the general range people work in:
| Source | Calcium chloride test | Relative humidity test |
|---|---|---|
| Ready mixed concrete association guidance | Limits generally specified at 3 to 5 pounds per 1,000 square feet per 24 hours | 75% to 80% typically targeted for floor coverings |
| Federal standard resinous flooring template (designer picks one or inserts another) | Maximum of 3 or 4.5 pounds per 1,000 square feet per 24 hours | Maximum of 75 percent |
| Federal fuel resistive thin film specification | No more than 3.0 pounds per 1,000 square feet per 24 hours; above 3.5 pounds, a moisture reducing system goes down first | Not stated in the parts read |
Those are reference points from the named sources, not a universal pass. The data sheet for the product going on your floor is the number that counts.
How many tests and where
The ready mixed concrete association's guidance is to "test at three random sample locations for areas up to 1000 ft2" and add one more for each additional 1,000 square feet. Tests are run at the building's normal service temperature and humidity, on a clean, dry surface. It also notes that slab-on-ground test results are only useful for timing a floor when the slab sits directly on an effective vapor retarder.
Both ASTM methods are careful about what a result means. The relative humidity method says results show the slab's condition "only at the time of the test and in the specific locations tested" (ASTM F2170), and the calcium chloride method says its result "may not indicate future conditions" (ASTM F1869). Test near the problem areas, test with the building running as it normally does, and keep the results with the job file.
When the slab fails the test
A failed test does not always mean no coating. The options, in the order the sources give them:
- Time and drying. Keep the slab at service conditions longer; heat and dehumidifiers speed drying (NRMCA CIP 28).
- A moisture mitigation system approved by the flooring or coating manufacturer, applied before the coating. The federal thin film specification puts one down over shot blasted concrete when its test is above 3.5 pounds (UFGS 09 67 23.15). Manufacturers describe these systems as acting "as a barrier between the concrete and final floor finish" (Moisture Mitigation). Membrane-forming moisture mitigation even has its own ASTM practice, written for resilient flooring rather than coatings, which says that when results come back too high, "one option is to apply a topical treatment to the concrete substrate surface" (ASTM F3010).
- A breathable coating or a different floor, which the association lists as the alternative.
Ask that the quote say which of these applies if the test fails, so the price is not a surprise. A slab that was coated without a test and then failed is covered in our guide on why epoxy floors peel or bubble, and recoating after a failure is on our repair and recoating page.
New concrete: how long to wait
The association says "it can take weeks to months in favorable interior ambient conditions for a concrete slab to dry to a level considered acceptable", and that in most cases newly placed slabs "cannot dry fast enough" to meet flooring and coating makers' moisture requirements, a problem that fast-track schedules make worse. Drying speed depends on the mix water, the concrete type, the slab thickness, the type of curing, and the room's temperature and humidity.
The federal specifications set their own floors for their own systems: one will not start a troweled topping "until the concrete has cured a minimum of 28 calendar days" (UFGS 09 67 23.13), and the thin film specification tests new slabs about 60 days after the pour. A cured slab and a dry slab are not the same thing; the test decides.
Moisture testing questions
Which moisture test is better, calcium chloride or relative humidity?
They measure different things, and the coating manufacturer says which one it accepts. The calcium chloride test reads vapor leaving the surface and only shallow moisture; the probe test reads humidity inside the slab. Some specifications accept either, with a separate limit for each.
Is taping plastic to the floor a real moisture test?
It is a screening check, not a pass. Moisture under the sheet is a warning sign, but the concrete industry's guidance says a dry result is not an assurance that the slab is dry below the surface.
How long does moisture testing take?
Roughly 60 to 72 hours once the test is set, by the published methods. The ready mixed concrete association describes 60 to 72 hours for the calcium chloride test and 72 hours of equilibrium in the hole for the probe test, and the building should be at service conditions before testing starts.
Can a floor be coated if it fails?
Sometimes, with a moisture mitigation system the coating manufacturer approves, applied before the coating. Other options are more drying time, or a breathable coating or a different floor.
Sources
- ASTM International, F2170, Standard Test Method for Determining Relative Humidity in Concrete Floor Slabs Using in situ Probes, read 2026-11-28
- ASTM International, F1869, Standard Test Method for Measuring Moisture Vapor Emission Rate of Concrete Subfloor Using Anhydrous Calcium Chloride, read 2026-11-28
- ASTM International, D4263, Standard Test Method for Indicating Moisture in Concrete by the Plastic Sheet Method, read 2026-11-28
- ASTM International, F3010, Standard Practice for Two-Component Resin Based Membrane-Forming Moisture Mitigation Systems for Use Under Resilient Floor Coverings, read 2026-11-28
- National Ready Mixed Concrete Association, CIP 28, Concrete Slab Moisture, 2017, read 2026-11-28
- American Concrete Institute, PRC-302.2-22, Concrete Slabs that Receive Moisture-Sensitive Flooring Materials: Guide (public preview), read 2026-11-28
- Unified Facilities Guide Specifications, Section 09 67 23.13, Standard Resinous Flooring, November 2019, read 2026-11-28
- Unified Facilities Guide Specifications, Section 09 67 23.15, Fuel Resistive Resinous Flooring, 3-Coat System, February 2021, read 2026-11-28
- Sherwin-Williams High Performance Flooring, Moisture Mitigation, read 2026-11-28
Tell us what you know about your slab
If you have moisture results, the age of the slab or a history of peeling, include them with your photos. For what happens to the slab before coating, see concrete floor preparation for epoxy, and for getting the building ready, see how to prepare a building for floor coating. Get a Quote